Short answer: "anodized" and "powder coated" are not specifications. A usable callout names the process class, the film thickness, the colour reference, the faces to be masked, and the acceptance test. Without those five, two suppliers will quote two different parts and both will claim to have met the drawing.
How to call out anodizing
A complete anodizing note looks like this:
- Process and class: sulfuric anodize to MIL-A-8625 Type II, Class 1 (dyed) or Class 2 (clear). Type III hard anodize when wear resistance matters, at 25–50 µm.
- Film thickness: 5–25 µm for Type II. State whether the range is a minimum, a nominal, or a maximum — a maximum matters on fits.
- Colour: a physical standard or a dyed reference, not a word like "black". Black dyes vary by lot.
- Sealing: sealed for corrosion resistance, unsealed only where a subsequent bond or conductive contact requires it.
- Masked areas: every face that must stay conductive or must stay within tolerance.
How to call out powder coating
- Chemistry: polyester for outdoor UV exposure, epoxy for chemical resistance indoors, epoxy-polyester hybrid for general use.
- Film build: 60–120 µm is the normal band. Specify minimum and maximum, because the maximum is what closes your bores.
- Colour and gloss: RAL or Pantone reference plus a gloss unit target. "Matte" alone is not measurable.
- Cure: 180–200 °C. Flag any press-fit insert, bonded magnet, or heat-sensitive component that cannot take that.
- Masking: a drawing view showing every masked face, including threads, bores, mating flanges and ground points.
Why masking is the line item people forget
Anodizing adds a few microns; powder coating adds 60–120 µm per surface, so a coated Ø10 mm bore closes by up to 0.24 mm. Threads fill, connector shoulders will not seat, and a grounding stud loses contact. Masking solves all three, but it is hand labour applied to every part in the run.
Put the masked faces on the drawing at quotation stage. A masking requirement discovered after tooling is a permanent cost increase on the programme.
Holding colour across a production run
Colour is where aluminium finishes most often fail inspection, and it is decided before the finish shop sees the part:
- Alloy and billet. 6063 anodises brighter and more uniformly than 6061; alloying content shifts the final tone. We run primary 6063, ceramic-filtered and homogenised, for cosmetic parts.
- One dye lot. Anodising colour is set per dye bath, so a run split across two baths will show a seam.
- Measurement, not opinion. Each batch is checked with a spectrophotometer against the approved first article, and ΔE is the acceptance number.
- Powder batches. Powder is more forgiving, but a mid-run batch change is still visible on adjacent panels.
How to inspect what you specified
- Film thickness: eddy-current gauge, several readings per face, against the drawing range.
- Corrosion: neutral salt spray hours. A pretreated powder coat commonly passes 500+ hours; sealed Type II anodizing is specified by hours appropriate to the environment, not by a universal number.
- Adhesion: cross-hatch or impact test for powder; for anodizing, a dye-stain or abrasion check on the sealed film.
- Colour: spectrophotometer against the approved sample, ΔE within the agreed limit.
Two specifications that cause rework
- "Anodize per sample" with no film thickness or class. The sample may have been Type II at 12 µm; the next shop runs Type III at 40 µm and the bore no longer takes the connector.
- Powder coat over an unmasked ground face. The enclosure arrives looking correct and fails EMC in the chamber, which is the most expensive place to discover a finish problem.
FAQ
Does anodizing change part dimensions?
Yes, by roughly half the film thickness per face — a 10 µm film grows about 5 µm outward. On a ±0.05 mm fit this is usually tolerable; on a press fit it should be called out.
Can I anodize and then powder coat?
You can, but there is little reason to. The powder will not adhere usefully to a sealed anodic film, and the anodizing underneath adds cost without benefit. Choose one per face, mask the rest.
What is the maximum film I should specify?
Only what the environment needs. Thicker films crack at tight bend radii and cost more; a 20 µm Type II is enough for most indoor enclosures.