Why finish defects only appear after anodising
An anodised aluminium enclosure is unforgiving: the oxide layer is transparent, so anything wrong in the substrate — a weld line, a sand hole, a scuff from handling — shows up as a visible defect, not a hidden one. That is why we judge finish quality on the billet and the process, not on a final polish. This note lists the defects overseas buyers ask about most and where each one actually originates.
The four defects we see most
- Sand holes and pinholes — small voids that open up as dark specks once anodised.
- Streaks and colour bands — uneven dye take-up across one face or between batches.
- Weld lines — a faint line where the metal re-joins inside a semi-hollow die.
- Scuffs and die lines — handling marks and longitudinal lines from the die bearing.
Where each defect originates
| Defect | Root cause | Prevention |
|---|---|---|
| Sand holes / pinholes | Recycled or poorly degassed billet; gas trapped in the metal | Primary billet from state-owned mills, ceramic-filtered on-line |
| Streaks / colour bands | Inconsistent billet composition or uneven anodising current | Homogenised billet; spectrophotometer check against the first article |
| Weld lines | Port-hole die where the metal re-joins under pressure | Keep weld lines off cosmetic and sealing faces by die design |
| Scuffs / die lines | Handling or worn die bearing | Protective packing; bearing maintenance and first-article inspection |
How to prevent defects at design stage
- Name the alloy and temper on the drawing — 6063-T5/T6 is our default for cosmetic enclosures because it takes the most even anodised colour.
- Keep sharp internal corners out of cosmetic faces; they anodise unevenly.
- Locate weld lines deliberately — tell us which faces are seen and we will route the line away from them.
- Decide the finish before the die is cut, since masking and groove geometry are set at tooling stage.
If a finish defect reaches you, our quality process records it per batch and resolves it by re-anodising or replacement. Send a photo and the batch reference and we will trace it. To discuss a finish-critical part, start with a free DFM review and tell us which faces are cosmetic.